ГОСТ Р9М4К8

Location » Home » Grades > Special Alloy > Р9М4К8

Grades | Special Alloy | Р9М4К8

ГОСТ Р9М4К8

Print

Р9М4К8 Application:Carbide for cutting tools

Chemical composition(mass fraction)(wt.%) of the Р9М4К8
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Ni(%) Mo(%) V(%) W(%) Cu(%) Co(%)
1.00-1.10 0.20-0.50 0.20-0.50 ≤0.030 ≤0.030 7.50-8.50 2.30-2.70 3.80-4.30 2.30-2.70 2.30-2.70 ≤0.25 7.50-8.50

Mechanical properties of grade Р9М4К8

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
852 (≥) 577 (≥) 13 33 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 121

Physical properties of grade Р9М4К8

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
269 (≥) 849 (≥) 33 13 34 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
261 226 889 - - -

Р9М4К8 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED