BT4

Location » Home » Grades > Special Alloy > BT4

Grades | Special Alloy | BT4

BT4

Print

BT4 Application:Carbide for cutting tools

Chemical composition(mass fraction)(wt.%) of the BT4
C(%) Si(%) Mn(%) Cr(%) Ni(%) Mo(%) V(%) W(%) Co(%) Other(%)
0.75-0.85 ≤0.40 ≤0.40 3.75-4.50 ≤0.40 ≤1.00 1.75-2.05 18.5-19.5 9.00-10.0 Cu≤0.20,Sn≤0.05

Mechanical properties of grade BT4

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
694 (≥) 849 (≥) 43 31 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 321

Physical properties of grade BT4

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
263 (≥) 548 (≥) 43 41 42 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
458 537 127 - - -

BT4 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED