ISO ISO X53CrMnNiNbN21 9

Location » Home » Grades > Special Alloy > ISO X53CrMnNiNbN21 9

Grades | Special Alloy | ISO X53CrMnNiNbN21 9

ISO ISO X53CrMnNiNbN21 9

Print

ISO X53CrMnNiNbN21 9 Application:ISO standard valve austenite steel

Chemical composition(mass fraction)(wt.%) of the ISO X53CrMnNiNbN21 9
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Ni(%) W(%) N(%) Other(%)
0.48-0.58 Max 0.45 8.00-10.0 Max 0.05 Max 0.03 20.0-22.0 3.25-4.50 0.80-1.50 0.38-0.50 C+N≥0.90,Nb+Ta 2.00-3.00

Mechanical properties of grade ISO X53CrMnNiNbN21 9

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
938 (≥) 854 (≥) 34 21 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 411

Physical properties of grade ISO X53CrMnNiNbN21 9

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
682 (≥) 329 (≥) 21 44 43 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
877 635 773 - - -

ISO X53CrMnNiNbN21 9 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED