STS316L Application:KS standard austenite stainless steel bars(KS D3706-1992)

Chemical composition(mass fraction)(wt.%) of the STS316L
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Ni(%) Mo(%)
Max O.030 Max 1.00 Max 2.00 Max 0.045 Max 0.03 16.0-18.0 12.00-15.00 2.00-3.00

Mechanical properties of grade STS316L

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
318 (≥) 388 (≥) 23 11 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 413

Physical properties of grade STS316L

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
524 (≥) 778 (≥) 32 24 32 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
571 166 691 - - -

STS316L Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED