SS SS 2382

Location » Home » Grades > Special Alloy > SS 2382

Grades | Special Alloy | SS 2382

SS SS 2382

Print

SS 2382 Application:Swedish SS standard stainless steel and heat resistant steel

Chemical composition(mass fraction)(wt.%) of the SS 2382
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Ni(%) Mo(%) Ti(%)
Max 0.030 Max 1.0 Max 0.5 Max 0.03 0.15-0.35 17.5-18.5 Max 1.0 2.0-2.5 0.30-1.00

Mechanical properties of grade SS 2382

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
156 (≥) 565 (≥) 12 11 13 Solution and Aging, Annealing, Ausaging, Q+T,etc 331

Physical properties of grade SS 2382

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
731 (≥) 116 (≥) 31 31 14 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
463 721 939 - - -

SS 2382 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED