CSN 419315

Location » Home » Grades > Special Alloy > 419315

Grades | Special Alloy | 419315

CSN 419315

Print

419315 Application:The Czech republic tool steel

Chemical composition(mass fraction)(wt.%) of the 419315
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) V(%) W(%)
0.80-0.90 0.15-0.35 1.80-2.10 0.030 0.035 0.20 ~0.40 0.10-0.20 0.40-0.60

Mechanical properties of grade 419315

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
634 (≥) 856 (≥) 31 21 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 324

Physical properties of grade 419315

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
834 (≥) 243 (≥) 42 34 23 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
177 264 212 - - -

419315 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED