GBT GH2135

Location » Home » Grades > Special Alloy > GH2135

Grades | Special Alloy | GH2135

GBT GH2135

Print

GH2135 Application:Age hardening type iron base alloy

Chemical composition(mass fraction)(wt.%) of the GH2135
C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Ni(%) Mo(%) W(%) Al(%) Ti(%) Other(%)
≤0.08 0.5 0.4 0.02 0.02 14.0-16.0 33.0-36.0 1.70-2.20 1.70-2.20 2.00-2.80 2.10-2.50 B≤0.015,Ce≤0.03

Mechanical properties of grade GH2135

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
563 (≥) 273 (≥) 43 41 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 131

Physical properties of grade GH2135

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
383 (≥) 537 (≥) 44 22 44 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
958 991 662 - - -

GH2135 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED