Grades | Stainless Steels | PH 15-7 Mo

UNS PH 15-7 Mo ( Precipitation-Hardening )

PDF | Word | Print

PH 15-7 Mo Application:Special Purpose Alloys ("Superalloys")

Chemical composition(mass fraction)(wt.%) of the PH 15-7 Mo
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.07
Si - 0.30
Mn - 0.50
Cr - 15.00
Ni - 7.00
Mo - 2.20
Co - -
W - -
Al - 1.17
Cu - -
Ti - -
Fe - remaining

Mechanical properties of grade PH 15-7 Mo

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
539 (≥) 138 (≥) 44 23 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 313

Physical properties of grade PH 15-7 Mo

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
581 (≥) 573 (≥) 41 12 31 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
765 413 117 - - -

PH 15-7 Mo Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED