Grades | Stainless Steels | 1.4418

AFNOR 1.4418 ( Precipitation-Hardening )

PDF | Word | Print

1.4418 Application:Aerospace series - Steel FE-PM 3504 (X4CrNiMo16-5-1) - Air melted - Hardened and tempered - Bar - De = 200 mm - 900 MPa = Rm = 1 050 MPa

Chemical composition(mass fraction)(wt.%) of the 1.4418
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.06
Si - 0.70
Mn - 1.50
P - 0.040
S - 0.015
Cr 15.00 17.00
Mo 0.80 1.50
Ni 4.00 6.00
N 0.020 -

Mechanical properties of grade 1.4418

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
283 (≥) 828 (≥) 33 41 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 132

Physical properties of grade 1.4418

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
348 (≥) 743 (≥) 43 32 43 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
467 944 165 - - -

1.4418 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED