Grades | Stainless Steels | XM-19,NITRONIC 50®,UNS S20910
UNS XM-19,NITRONIC 50®,UNS S20910 ( Austenite )
PDF | Word | Print
XM-19,NITRONIC 50®,UNS S20910 Application:used for the production of chains, bolts, nuts, pumps, parts for installation of heat exchangers, springs, valve parts, fittings, flanges, valves, fittings in the petrochemical industry, chemical, nitric, nuclear, offshore, maritime industries and shipbui
| Elements | Min.(≥) | Max.(≤) | Similar | Remarks |
|---|---|---|---|---|
| C | - | 0.06 | ||
| Si | - | 1.00 | ||
| Mn | 4.00 | 6.00 | ||
| P | - | 0.04 | ||
| S | - | 0.03 | ||
| Cr | 20.5 | 23.5 | ||
| Ni | 11.5 | 13.5 | ||
| Mo | 1.50 | 3.00 | ||
| Nb | 0.10 | 0.30 | ||
| N | 0.20 | 0.40 | ||
| V | 0.10 | 0.30 |
| Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | HBW |
|---|---|---|---|---|---|---|
| 418 (≥) | 734 (≥) | 13 | 22 | 23 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 131 |
| Property | Density kg/dm3 |
Temperature T °C/F |
Specific heat J / kgK |
Thermal conductivity W/mK |
Electric resistance µΩ·cm |
|---|---|---|---|---|---|
| 589 (≥) | 679 (≥) | 44 | 13 | 33 | Solution and Aging, Annealing, Ausaging, Q+T,etc |
| Temp. °C/°F |
Creep strain limit (10000h) (Rp1,0) N/mm2 |
Creep rupture strength (10000h) (Rp1,0) N/mm2 |
- | - | - |
| 621 | 432 | 172 | - | - | - |
| Product type | Products | Dimension | Processes | Deliver Status |
|---|---|---|---|---|
| Plates / Sheets | Plates / Sheets | 0.08-200mm(T)*W*L | Forging, hot rolling and cold rolling | Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting |
| Steel Bar | Round Bar, Flat Bar, Square Bar | Φ8-1200mm*L | Forging, hot rolling and cold rolling, Cast | Black, Rough Turning, Shot Blasting, |
| Coil / Strip | Steel Coil /Steel Strip | 0.03-16.0x1200mm | Cold-Rolled & Hot-Rolled | Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting |
| Pipes / Tubes | Seamless Pipes/Tubes, Welded Pipes/Tubes | OD:6-219mm x WT:0.5-20.0mm | Hot extrusion, Cold Drawn, Welded | Annealed, Solution and Aging, Q+T, ACID-WASHED |